Warning: error_log(/home/sxlanshenasjx8lnann8sdhwern/wwwroot/en/caches/error_log.php): failed to open stream: Permission denied in /home/sxlanshenasjx8lnann8sdhwern/wwwroot/en/phpcms/libs/functions/global.func.php on line 929 Warning: error_log(/home/sxlanshenasjx8lnann8sdhwern/wwwroot/en/caches/error_log.php): failed to open stream: Permission denied in /home/sxlanshenasjx8lnann8sdhwern/wwwroot/en/phpcms/libs/functions/global.func.php on line 929 Ion exchange resin pretreatment method - Technology - Xi'an Lanshen Environmental Protection Technology Co.,

Technology

location: Home - Technology

Ion exchange resin pretreatment method

2016.11.22

Ion exchange resins for industrial products must be pretreated to remove excess solvents, oligomers, or other impurities in the resin, which may affect the exchange and effluent quality. It can also improve the stability of the resin to be transferred to the desired ionic form, and it can play the role of activated resin.

The new factory soon after the resin, must be repeatedly washed into the water for the water, and then according to the order of pretreatment.

For the long time of the resin, saturated salt water immersion treatment, after washing and then pretreatment.

For the pharmaceutical industry, the food industry, resin, according to special requirements for processing.

Pretreatment of a resin

The resin with water to clear water after immersed in 2-4%NaOH solution for 4-8 hours, exhausted lye, washing resin until the discharge water close to neutral; then 5%HCl for 4-8 hours, exhausted acid, rinse with water until neutral.

Pretreatment of anion resin (b)

Wash the resin with water after the water is clear, with 5%HCl soak 4-8 hours, put the acid solution, rinse with water to neutral, and then soak in 2-4%NaOH solution for 4-8 hours, put the lye, rinse with water to neutral stand-by.